Optical constants of HOYA - FD (Dense flint)
M-FD80

Wavelength: µm
 (0.360 – 1.550)  
 

Complex refractive index (n+ik)[ i ]


n   k   LogX   LogY   eV

Derived optical constants

Dispersion formula

$$n^2=2.761638-0.01132633λ^{2}+0.02865346λ^{-2}+0.001529038λ^{-4}-8.743577\text{×}10^{-05}λ^{-6}+1.496579\text{×}10^{-05}λ^{-8}$$

Conditions & Spec sheet

n_absolute: false
wavelength_vacuum: false
temperature: 20.0 °C
thermal_dispersion:
  - type: "Schott formula"
    coefficients: -8.15303e-06 0.0 0.0 0.0 0.0 0.0
nd: 1.68893
Vd: 31.16
glass_code: 689312
glass_status: standard
density: 3.26 g/cm3
thermal_expansion:
  - temperature_range: -30 70 °C
    coefficient: 1.15e-05 K-1
  - temperature_range: 20 300 °C
    coefficient: 1.43e-05 K-1
dPgF: 0.0115
climatic_resistance: 3.0
stain_resistance: 3.0
acid_resistance: 3.0

Comments

Glass for molded optics lens

References

HOYA Zemax catalog 2017-04-01 (obtained from http://www.hoya-opticalworld.com)

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

INFO

HOYA Corporation

Hoya Corporation is a Japanese company manufacturing optical products.

External links


Glass

External links