Optical constants of BAF10
BAF10 (HOYA)
Wavelength:
µm
(0.340 – 1.01398)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.7324621-0.01249046λ^{2}+0.018562334λ^{-2}+0.00099990536λ^{-4}-6.8388552\text{×}10^{-05}λ^{-6}+4.9257931\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 6.13489e-06 0.0 0.0 0.0 0.0 0.0 nd: 1.67003 Vd: 47.19 glass_code: 670472 glass_status: special density: 3.61 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 7.2e-06 K-1 - temperature_range: 20 300 °C coefficient: 8.6e-06 K-1 dPgF: 0.0007 climatic_resistance: 1.0 stain_resistance: 1.0 acid_resistance: 2.0
Comments
Not in a position to accept new order because of discontinuation.
References
HOYA Zemax catalog 2017-04-01 (obtained from http://www.hoya-opticalworld.com)
Data
INFO
HOYA Corporation
Hoya Corporation is a Japanese company manufacturing optical products.External links
- HOYA Corporation
- HOYA Group Optics DIvision
- HOYA Corporation USA Optics DIvision
- Hoya Corporation - Wikipedia
BAF10 optical glass
BAF10 is a very popular optical glass. Most glass makers produce this or very similar glass under slightly different names.BAF10 and similar glasses produced by different makers
Maker | Glass |
---|---|
Schott | N-BAF10 |
Hikari | E-BAF10 |
HOYA | BAF10 |
Ohara | S-BAH10 |
CDGM | H-ZBAF52 |