Optical constants of SUMITA - VC
K-VC91(M)
Wavelength:
µm
(0.350 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=3.4226561-0.014620569λ^{2}+0.037712137λ^{-2}+0.0019015089λ^{-4}-0.00011042813λ^{-6}+1.2477487\text{×}10^{-05}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -1.08e-06 1.12e-08 -9.02e-11 8.61e-07 1.32e-09 0.245 nd: 1.88175 Vd: 34.9 glass_code: 887350 density: 4.87 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 7.7e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 9.5e-06 K-1 dPgF: -0.0025 climatic_resistance: 1.0 acid_resistance: 1.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book