$$n^2=2.5429277-0.01031719λ^{2}+0.014356944λ^{-2}+0.00031433872λ^{-4}-1.0824341\text{×}10^{-05}λ^{-6}+6.8100892\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 2.39e-07 1.74e-08 -2.81e-10 4.14e-07 1.06e-09 0.188 nd: 1.60729 Vd: 59.5 glass_code: 607595 density: 3.5 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 7.1e-06 K-1 - temperature_range: 20 300 °C coefficient: 7.7e-06 K-1 dPgF: -0.0001 climatic_resistance: 3.0 acid_resistance: 5.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)