Optical constants of SUMITA - PSK (Dense phosphate crown)
K-PSK400(M)
Wavelength:
µm
(0.270 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.4983595-0.0073445422λ^{2}+0.012430575λ^{-2}+0.00026343152λ^{-4}-1.3169766\text{×}10^{-05}λ^{-6}+8.1753544\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -1.29e-05 6.41e-09 -4.23e-11 4.04e-07 7.68e-10 0.173 nd: 1.59179 Vd: 67.7 glass_code: 595678 density: 4.05 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 1.01e-05 K-1 - temperature_range: 20 300 °C coefficient: 1.29e-05 K-1 dPgF: 0.0127 climatic_resistance: 1.0 acid_resistance: 1.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book