Optical constants of SUMITA - PSK (Dense phosphate crown)
K-PSK300
Wavelength:
µm
(0.280 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.5225185-0.0094325814λ^{2}+0.012753583λ^{-2}+0.00028565036λ^{-4}-8.905806\text{×}10^{-06}λ^{-6}+2.8110143\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -1.33e-05 1.14e-08 -3e-11 4.03e-07 3.8e-10 0.173 nd: 1.59950 Vd: 65.6 glass_code: 600656 density: 3.49 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 1.05e-05 K-1 - temperature_range: 20 300 ℃ coefficient: 1.28e-05 K-1 dPgF: 0.0077 climatic_resistance: 2.0 acid_resistance: 4.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book