Optical constants of SUMITA - PSK (Dense phosphate crown)
K-PSK200
Wavelength:
µm
(0.290 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.5593395-0.0088787219λ^{2}+0.015115397λ^{-2}+0.0002035651λ^{-4}+7.5991137\text{×}10^{-06}λ^{-6}-1.5375246\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -3.04e-06 8.75e-09 -5.81e-11 5.61e-07 7.53e-10 0.187 nd: 1.61305 Vd: 59.0 glass_code: 613590 density: 3.38 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 1e-05 K-1 - temperature_range: 20 300 °C coefficient: 1.23e-05 K-1 dPgF: 0.0041 climatic_resistance: 1.0 acid_resistance: 4.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book