Optical constants of SUMITA - PSK (Dense phosphate crown)
K-PSK100
Wavelength:
µm
(0.320 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.4948235-0.0091228463λ^{2}+0.013721276λ^{-2}+0.00023830265λ^{-4}+4.1915859\text{×}10^{-06}λ^{-6}-3.8958137\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -8.26e-07 2.08e-08 -1.4e-10 5.32e-07 -2.69e-10 0.175 nd: 1.59170 Vd: 60.7 glass_code: 592607 density: 3.24 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 9.5e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 1.14e-05 K-1 dPgF: 0.0028 climatic_resistance: 1.0 acid_resistance: 6.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book