Optical constants of SUMITA - PSF
K-PSFn5
Wavelength:
µm
(0.370 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=3.4965005-0.011373234λ^{2}+0.059139817λ^{-2}+0.0031967827λ^{-4}-9.7424772\text{×}10^{-05}λ^{-6}+3.2744737\text{×}10^{-05}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 3.38e-06 2.43e-08 -2.21e-10 2.2e-06 1.89e-09 0.277 nd: 1.92110 Vd: 22.4 glass_code: 921224 density: 5.22 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 1.08e-05 K-1 - temperature_range: 20 300 °C coefficient: 1.12e-05 K-1 dPgF: 0.0185 climatic_resistance: 1.0 acid_resistance: 1.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book