Optical constants of SUMITA - PSF
K-PSFn2
Wavelength:
µm
(0.380 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=3.7699503-0.013004151λ^{2}+0.072310519λ^{-2}+0.0035123072λ^{-4}-1.0361594\text{×}10^{-05}λ^{-6}+3.8615781\text{×}10^{-05}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 8.11e-06 2.15e-08 -1.06e-10 2.16e-06 2.01e-09 0.291 nd: 2.00170 Vd: 20.6 density: 5.48 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 7.3e-06 K-1 - temperature_range: 20 300 °C coefficient: 9.2e-06 K-1 dPgF: 0.0257 climatic_resistance: 1.0 acid_resistance: 1.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book