Optical constants of SUMITA - PG
K-PG375(M)
Wavelength:
µm
(0.300 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.3359595-0.0077028465λ^{2}+0.011800095λ^{-2}+0.00020814746λ^{-4}-3.5241725\text{×}10^{-06}λ^{-6}+3.1241519\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -1.51e-05 1.45e-09 -9.02e-11 5.44e-07 3.99e-10 0.176 nd: 1.53922 Vd: 62.7 glass_code: 543629 density: 2.9 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 1.29e-05 K-1 - temperature_range: 20 300 ℃ coefficient: 1.6e-05 K-1 dPgF: 0.0053 climatic_resistance: 2.0 acid_resistance: 3.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book