Optical constants of SUMITA - PFK
K-PFK80(M)
Wavelength:
µm
(0.270 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.212796-0.0056313014λ^{2}+0.0083136801λ^{-2}+0.00015790111λ^{-4}-1.2884506\text{×}10^{-05}λ^{-6}+8.4786533\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -1.91e-05 -2.54e-09 -5.06e-11 3.29e-07 5.19e-11 0.188 nd: 1.49533 Vd: 80.8 glass_code: 497815 density: 3.6 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 1.34e-05 K-1 - temperature_range: 20 300 °C coefficient: 1.54e-05 K-1 dPgF: 0.0276 climatic_resistance: 1.0 acid_resistance: 3.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book