Optical constants of SUMITA - PBK
K-PBK50(M)
Wavelength:
µm
(0.270 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.2812358-0.010469171λ^{2}+0.010938493λ^{-2}+0.00025045867λ^{-4}-1.2796276\text{×}10^{-05}λ^{-6}+7.9827772\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 5.1e-08 2.09e-08 -1.11e-11 4.38e-07 5.79e-10 0.176 nd: 1.52025 Vd: 62.2 glass_code: 523623 density: 2.43 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 6.7e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 9.2e-06 K-1 dPgF: -0.0046 climatic_resistance: 2.0 acid_resistance: 4.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book