Optical constants of SUMITA - LaK (Lanthanum crown)
K-LaKn7
Wavelength:
µm
(0.340 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.735741-0.011476747λ^{2}+0.017975035λ^{-2}+0.00072020288λ^{-4}-5.1933951\text{×}10^{-05}λ^{-6}+3.5980087\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -2.14e-07 1.48e-08 -1.61e-10 5.55e-07 4.75e-10 0.191 nd: 1.67000 Vd: 51.7 glass_code: 670517 density: 3.78 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 6.3e-06 K-1 - temperature_range: 20 300 °C coefficient: 8.5e-06 K-1 dPgF: -0.0042 climatic_resistance: 1.0 acid_resistance: 5.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book