Optical constants of SUMITA - LaFK
K-LaFK65
Wavelength:
µm
(0.270 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.7016579-0.011617767λ^{2}+0.015597681λ^{-2}+0.00019111207λ^{-4}+1.132323\text{×}10^{-05}λ^{-6}-5.9630893\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -7.58e-06 9.42e-09 -3.47e-11 3.97e-07 4.24e-10 0.182 nd: 1.65670 Vd: 62.3 glass_code: 657623 density: 4.36 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 8.1e-06 K-1 - temperature_range: 20 300 °C coefficient: 1.03e-05 K-1 dPgF: 0.0026 climatic_resistance: 1.0 acid_resistance: 5.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book