Optical constants of SUMITA - GIR
K-GIR140
Wavelength:
µm
(0.280 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.9854628-0.0065859032λ^{2}+0.026407911λ^{-2}+0.00084695423λ^{-4}-3.2505558\text{×}10^{-05}λ^{-6}+3.1878545\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 5.13e-06 1.39e-08 -3.39e-10 9.92e-07 9.74e-10 0.216 nd: 1.75106 Vd: 43.1 glass_code: 751431 density: 5.24 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 5.9e-06 K-1 - temperature_range: 20 300 °C coefficient: 9.7e-06 K-1 dPgF: -0.004 climatic_resistance: 1.0 acid_resistance: 4.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book