Optical constants of SUMITA - GFK
K-GFK70
Wavelength:
µm
(0.280 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.4293935-0.0057591097λ^{2}+0.011512013λ^{-2}+0.0001324924λ^{-4}+7.3250033\text{×}10^{-06}λ^{-6}-5.7195445\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -2.47e-05 -1.68e-09 -2.49e-11 3.77e-07 3.45e-10 0.178 nd: 1.56907 Vd: 71.3 glass_code: 569713 density: 4.46 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 1.32e-05 K-1 - temperature_range: 20 300 °C coefficient: 1.56e-05 K-1 dPgF: 0.0207 climatic_resistance: 1.0 acid_resistance: 1.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book