Optical constants of SUMITA - CaFK
K-CaFK95(M)
Wavelength:
µm
(0.270 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.0377918-0.0045854882λ^{2}+0.0057460341λ^{-2}+0.00014824175λ^{-4}-1.2924899\text{×}10^{-05}λ^{-6}+6.7640906\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -2.06e-05 -5.62e-09 -2.69e-11 3.17e-07 3.49e-10 0.174 nd: 1.43312 Vd: 95.0 glass_code: 434950 density: 3.54 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 1.29e-05 K-1 - temperature_range: 20 300 °C coefficient: 1.67e-05 K-1 dPgF: 0.0506 climatic_resistance: 1.0 acid_resistance: 4.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book