Optical constants of SUMITA - BaSF (Barium dense flint)
K-BaSF5
Wavelength:
µm
(0.340 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.5165762-0.01183779λ^{2}+0.017631594λ^{-2}+0.00095834052λ^{-4}-6.7623905\text{×}10^{-05}λ^{-6}+6.2543393\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -1.33e-06 1.61e-08 -2.3e-10 5.78e-07 6.96e-10 0.262 nd: 1.60323 Vd: 42.5 glass_code: 603425 density: 2.71 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 7.9e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 1.02e-05 K-1 dPgF: 0.0005 climatic_resistance: 2.0 acid_resistance: 3.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book