Optical constants of SUMITA - BaF (Barium flint)
K-BaFn1
Wavelength:
µm
(0.330 – 2.000)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.7669297-0.011669996λ^{2}+0.02151984λ^{-2}+0.00070810281λ^{-4}-2.495822\text{×}10^{-05}λ^{-6}+3.7747946\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -8.23e-07 1.72e-08 -1.68e-10 5.4e-07 8.98e-10 0.251 nd: 1.68250 Vd: 44.5 glass_code: 683445 density: 3.62 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 7.3e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 8.4e-06 K-1 dPgF: -0.0003 climatic_resistance: 1.0 acid_resistance: 4.0
References
SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book