Optical constants of SUMITA - BaF (Barium flint)
K-BaF9

Wavelength: µm
 (0.350 – 2.000)  
 

Complex refractive index (n+ik)[ i ]


n   k   LogX   LogY   eV

Derived optical constants

Dispersion formula

$$n^2=2.6455399-0.010990833λ^{2}+0.018955207λ^{-2}+0.00040800743λ^{-4}+9.934634\text{×}10^{-06}λ^{-6}+9.3197902\text{×}10^{-07}λ^{-8}$$

Conditions & Spec sheet

n_absolute: false
wavelength_vacuum: false
temperature: 20.0 ℃
thermal_dispersion:
  - type: "Schott formula"
    coefficients: -4.02e-07 1.44e-08 -1.41e-10 4.98e-07 5.81e-10 0.243
nd: 1.64328
Vd: 47.8
glass_code: 643478
density: 3.44 g/cm3
thermal_expansion:
  - temperature_range: -30 70 ℃
    coefficient: 6.6e-06 K-1
  - temperature_range: 20 300 ℃
    coefficient: 8.2e-06 K-1
dPgF: 0.0012
climatic_resistance: 1.0
acid_resistance: 2.0

References

SUMITA Zemax catalog 2017-02-02 (obtained from http://www.sumita-opt.co.jp)
See also SUMITA optical glass data book

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

INFO

SUMITA Optical Glass, Inc.

SUMITA Optical Glass, Inc. is a Japanese glass manufacturer

External links


Glass

External links