Optical constants of SCHOTT - SF (Dense flint)
SF14
Wavelength:
µm
(0.39 – 2.5)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.69182538λ^2}{λ^2-0.0133151542}+\frac{0.285919934λ^2}{λ^2-0.0612647445}+\frac{1.12595145λ^2}{λ^2-118.405242}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 8.85e-06 1.81e-08 -4.12e-11 1.39e-06 1.53e-09 0.279 nd: 1.76182 Vd: 26.53 glass_code: 762265.454 glass_status: preferred density: 4.54 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 6.6e-06 K-1 - temperature_range: 20 300 °C coefficient: 7.4e-06 K-1 dPgF: 0.0134 climatic_resistance: 1.0 stain_resistance: 0.0 acid_resistance: 1.0 alkali_resistance: 1.2 phosphate_resistance: 1.0
Comments
was replaced by N-SF14
References
SCHOTT Zemax catalog 2017-01-20b (obtained from http://www.schott.com)
See also SCHOTT glass data sheets