Optical constants of SCHOTT - SF (Dense flint)
SF10
Wavelength:
µm
(0.38 – 2.5)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.61625977λ^2}{λ^2-0.0127534559}+\frac{0.259229334λ^2}{λ^2-0.0581983954}+\frac{1.07762317λ^2}{λ^2-116.60768}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 5.31e-06 1.59e-08 -4.07e-11 1.28e-06 1.32e-09 0.27 nd: 1.72825 Vd: 28.41 glass_code: 728284.428 glass_status: standard density: 4.28 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 7.5e-06 K-1 - temperature_range: 20 300 °C coefficient: 8.4e-06 K-1 dPgF: 0.0085 climatic_resistance: 1.0 stain_resistance: 0.0 acid_resistance: 1.0 alkali_resistance: 1.2 phosphate_resistance: 2.0
Comments
lead containing glass type
References
SCHOTT Zemax catalog 2017-01-20b (obtained from http://www.schott.com)
See also SCHOTT glass data sheets
Data
INFO
SF10 optical glass
SF10 is a popular optical glass. Most glass makers produce this or very similar glass under slightly different names.SF10 and similar glasses produced by different makers
Maker | Glass |
---|---|
Schott | N-SF10 |
Hikari | E-SF10 |
HOYA | E-FD10 |
Sumita | K-SFLD10 |
CDGM | ZF4 |