Optical constants of SCHOTT - SF (Dense flint)
N-SF56
Wavelength:
µm
(0.38 – 2.5)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.73562085λ^2}{λ^2-0.0129624742}+\frac{0.317487012λ^2}{λ^2-0.0612884288}+\frac{1.95398203λ^2}{λ^2-161.559441}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -4.13e-06 7.65e-09 -1.12e-11 9.9e-07 1.57e-09 0.287 nd: 1.7847 Vd: 26.1 glass_code: 785261.328 glass_status: special density: 3.28 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 8.7e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 1e-05 K-1 dPgF: 0.014 climatic_resistance: 1.0 stain_resistance: 0.0 acid_resistance: 1.0 alkali_resistance: 1.3 phosphate_resistance: 1.0
Comments
inquiry glass
References
SCHOTT Zemax catalog 2017-01-20b (obtained from http://www.schott.com)
See also SCHOTT glass data sheets