Optical constants of SCHOTT - SF (Dense flint)
N-SF19
Wavelength:
µm
(0.37 – 2.5)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.52005444λ^2}{λ^2-0.01096144}+\frac{0.17573947λ^2}{λ^2-0.0593248486}+\frac{1.43623424λ^2}{λ^2-126.795151}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 1.32e-06 1.22e-08 -1.36e-11 7.64e-07 1.09e-09 0.279 nd: 1.66679 Vd: 33.12 glass_code: 667331.290 glass_status: special density: 2.9 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 7.2e-06 K-1 - temperature_range: 20 300 °C coefficient: 8.3e-06 K-1 dPgF: 0.0095 climatic_resistance: 1.0 stain_resistance: 0.0 acid_resistance: 1.0 alkali_resistance: 1.2 phosphate_resistance: 1.0
Comments
inquiry glass
References
SCHOTT Zemax catalog 2017-01-20b (obtained from http://www.schott.com)
See also SCHOTT glass data sheets