Optical constants of SCHOTT - LaF (Lanthanum flint)
N-LAF32
Wavelength:
µm
(0.35 – 2.5)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.91731106λ^2}{λ^2-0.00978600358}+\frac{0.224019825λ^2}{λ^2-0.0386141473}+\frac{1.22087075λ^2}{λ^2-84.6431265}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 3.8e-06 1.1e-08 -1.83e-11 6.37e-07 8.03e-10 0.196 nd: 1.79457E+00 Vd: 4.55300E+01 glass_code: 795455.433 glass_status: preferred density: 4.325 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 5.89e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 6.98e-06 K-1 dPgF: -0.0075 climatic_resistance: 1.0 stain_resistance: 1.0 acid_resistance: 51.2 alkali_resistance: 1.0 phosphate_resistance: 2.0
References
SCHOTT Zemax catalog 2017-01-20b (obtained from http://www.schott.com)
See also SCHOTT glass data sheets