Optical constants of SCHOTT - FK (Fluor crown)
N-FK51
Wavelength:
µm
(0.29 – 2.5)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.971247817λ^2}{λ^2-0.00472301995}+\frac{0.216901417λ^2}{λ^2-0.0153575612}+\frac{0.904651666λ^2}{λ^2-168.68133}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -1.83e-05 -7.89e-09 -1.63e-12 3.74e-07 3.46e-10 0.15 nd: 1.48656 Vd: 84.47 glass_code: 487845.366 glass_status: preferred density: 3.66 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 1.33e-05 K-1 - temperature_range: 20 300 ℃ coefficient: 1.549e-05 K-1 dPgF: 0.0342 climatic_resistance: 2.0 stain_resistance: 0.0 acid_resistance: 52.3 alkali_resistance: 2.2 phosphate_resistance: 4.3
Comments
was replaced by N-FK51A
References
SCHOTT Zemax catalog 2017-01-20b (obtained from http://www.schott.com)