Optical constants of SCHOTT - FK (Fluor crown)
FK3
Wavelength:
µm
(0.3 – 2.5)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.973346627λ^2}{λ^2-0.00640795469}+\frac{0.146642231λ^2}{λ^2-0.020565293}+\frac{0.679304225λ^2}{λ^2-80.4965389}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -4.9e-06 1.23e-08 -1.19e-10 3.45e-07 7.72e-10 0.18 nd: 1.4645 Vd: 65.77 glass_code: 464658.227 glass_status: special density: 2.27 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 8.2e-06 K-1 - temperature_range: 20 300 °C coefficient: 9.4e-06 K-1 dPgF: -0.0003 climatic_resistance: 2.0 stain_resistance: 3.0 acid_resistance: 52.4 alkali_resistance: 2.0 phosphate_resistance: 1.0
Comments
inquiry glass
References
SCHOTT Zemax catalog 2017-01-20b (obtained from http://www.schott.com)
See also SCHOTT glass data sheets