Optical constants of SCHOTT - BaF (Barium flint)
N-BAF3
Wavelength:
µm
(0.365 – 2.5)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.34859634λ^2}{λ^2-0.00871492932}+\frac{0.10764424λ^2}{λ^2-0.0478406436}+\frac{1.13207084λ^2}{λ^2-112.936116}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 1.4e-06 1.24e-08 -9.39e-12 5.91e-07 7.44e-10 0.235 nd: 1.58272 Vd: 46.64 glass_code: 583466.279 glass_status: special density: 2.792 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 7.17e-06 K-1 - temperature_range: 20 300 °C coefficient: 8.24e-06 K-1 dPgF: 0.0015 climatic_resistance: 1.0 stain_resistance: 0.0 acid_resistance: 1.0 alkali_resistance: 1.0 phosphate_resistance: 1.0
Comments
inquiry glass
References
SCHOTT Zemax catalog 2017-01-20b (obtained from http://www.schott.com)
See also SCHOTT glass data sheets