Optical constants of SCHOTT - BaF (Barium flint)
BAFN6
Wavelength:
µm
(0.35 – 2.325)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.36719201λ^2}{λ^2-0.00882820704}+\frac{0.10907994λ^2}{λ^2-0.0438731646}+\frac{1.02108011λ^2}{λ^2-113.58602}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 1.34e-06 1.34e-08 -5.5e-11 4.95e-07 3.62e-10 0.265 nd: 1.589 Vd: 48.45 glass_code: 589485.317 glass_status: special density: 3.17 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 7.8e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 8.5e-06 K-1 dPgF: 0.0002 climatic_resistance: 2.0 stain_resistance: 0.0 acid_resistance: 2.0 alkali_resistance: 2.0 phosphate_resistance: 1.0
Comments
inquiry glass
References
SCHOTT Zemax catalog 2017-01-20b (obtained from http://www.schott.com)
See also SCHOTT glass data sheets