Optical constants of OHARA - PBH (Plumbate, high-index)
PBH72
Wavelength:
µm
(0.3 – 2.4)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=3.4684938-0.010731638λ^{2}+0.058252246λ^{-2}+0.0046536748λ^{-4}-0.0003034305λ^{-6}+4.8216298\text{×}10^{-05}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 2.001e-05 0.0 0.0 0.0 0.0 0.0 nd: 1.915356 Vd: 21.171926 glass_code: 915212 glass_status: preferred density: 5.97 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 8.8e-06 K-1 - temperature_range: 20 300 °C coefficient: 9.6e-06 K-1 dPgF: 0.022 acid_resistance: 53.4 phosphate_resistance: 4.2
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets