Optical constants of OHARA - PBH (Plumbate, high-index)
PBH56
Wavelength:
µm
(0.36 – 2.4)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.78552677λ^2}{λ^2-0.0136046011}+\frac{0.446684871λ^2}{λ^2-0.0570875152}+\frac{1.21749317λ^2}{λ^2-129.967536}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 7.53e-06 1.29e-08 -3.4e-11 1.93e-06 1.53e-09 0.268 nd: 1.841390 Vd: 24.559059 glass_code: 841246 glass_status: special density: 5.35 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 8.4e-06 K-1 - temperature_range: 20 300 °C coefficient: 9.6e-06 K-1 dPgF: 0.011
Comments
Improved XMT at 365
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)