Optical constants of OHARA - PBH (Plumbate, high-index)
PBH3W
Wavelength:
µm
(0.3 – 2.4)
Derived optical constants
n
k
logX
logY
eV
Dispersion formula
$$n^2=2.9157717-0.0100817λ^{2}+0.03409894λ^{-2}+0.0021965014λ^{-4}-0.00012386955λ^{-6}+1.5766843\text{×}10^{-05}λ^{-8}$$Conditions & Spec sheet
n_is_absolute: false λ_is_vacuum: false temperature: 25.0 °C coefficients_of_thermal_dispersion: 1.163e-05 0.0 0.0 0.0 0.0 0.0 n_d: 1.739998 V_d: 28.287409 glass_code: 740283 glass_status: preferred density: 4.66 g/cm3 coefficient_of_thermal_expansion_1: 8.2e-06 K-1 coefficient_of_thermal_expansion_2: 9.2e-06 K-1 ΔP_gF: 0.006 acid_resistance: 3.2 phosphate_resistance: 3.0
Comments
Improved Transmittance
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets