Optical constants of OHARA - NSL (Niobosilicate, low-index)
S-NSL2
Wavelength:
µm
(0.3 – 2.4)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.951239368λ^2}{λ^2-0.00513091895}+\frac{0.313094652λ^2}{λ^2-0.0231960516}+\frac{1.70928507λ^2}{λ^2-201.539573}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 ℃ nd: 1.516016 Vd: 56.858179 glass_code: 516568 glass_status: preferred density: 2.47 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 8.8e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 1.08e-05 K-1 dPgF: -0.0016 acid_resistance: 1.0 phosphate_resistance: 1.0
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets