Optical constants of OHARA - NSL (Niobosilicate, low-index)
NSL33
Wavelength:
µm
(0.3 – 2.4)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.2582399-0.0079875836λ^{2}+0.012575688λ^{-2}+0.00022130477λ^{-4}+1.0685962\text{×}10^{-06}λ^{-6}+3.9764383\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 1.239e-06 0.0 0.0 0.0 0.0 0.0 nd: 1.514536 Vd: 54.714595 glass_code: 515547 glass_status: preferred density: 2.6 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 9.1e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 1.07e-05 K-1 dPgF: -0.0021 acid_resistance: 1.0 phosphate_resistance: 1.0
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets