Optical constants of OHARA - LAH (Lanthanum, high-index)
LAH80
Wavelength:
µm
(0.3 – 2.4)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{2.06636247λ^2}{λ^2-0.0122133846}+\frac{0.349315832λ^2}{λ^2-0.0555959908}+\frac{1.91746463λ^2}{λ^2-125.47362}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 2.6e-06 1.15e-08 -3.36e-11 8.82e-07 1.2e-09 0.279 nd: 1.885000 Vd: 30.163795 glass_code: 885302 glass_status: special density: 3.99 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 6.6e-06 K-1 - temperature_range: 20 300 °C coefficient: 8.2e-06 K-1 dPgF: 0.0052 climatic_resistance: 2.0 acid_resistance: 2.3 phosphate_resistance: 1.0
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets