$$n^2-1=\frac{2.11102709λ^2}{λ^2-0.0120714135}+\frac{0.370368094λ^2}{λ^2-0.0532464416}+\frac{1.62687484λ^2}{λ^2-109.166396}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 2.69e-06 1.07e-08 -9.48e-12 8.91e-07 1.11e-09 0.274 nd: 1.902699 Vd: 31.005320 density: 4.9 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 6.1e-06 K-1 dPgF: 0.003 climatic_resistance: 3.0 acid_resistance: 4.2 phosphate_resistance: 2.0