Optical constants of OHARA - LAH (Lanthanum, high-index)
L-LAH53
Wavelength:
µm
(0.34 – 0.7)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.87409991λ^2}{λ^2-0.00993318344}+\frac{0.297921402λ^2}{λ^2-0.0405501825}+\frac{1.35064285λ^2}{λ^2-100.5022}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 7.31e-06 1.04e-08 -8.93e-12 7.66e-07 7.96e-10 0.229 nd: 1.806249 Vd: 40.907302 glass_code: 806409 density: 4.49 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 5.9e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 7.2e-06 K-1 dPgF: -0.0065 climatic_resistance: 1.0 acid_resistance: 51.2 phosphate_resistance: 2.0
Comments
Low Softening Temperature
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets