Optical constants of OHARA - BSM (Borosilicate, medium-index)
S-BSM36
Wavelength:
µm
(0.3 – 0.7)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.6546711-0.012819365λ^{2}+0.015197193λ^{-2}+0.00050420821λ^{-4}-3.4995634\text{×}10^{-05}λ^{-6}+2.0492682\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -7.36e-07 1.43e-08 -2.88e-12 5.38e-07 1.11e-09 0.119 nd: 1.642495 Vd: 58.369399 glass_code: 643584 glass_status: special density: 3.64 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 6.4e-06 K-1 - temperature_range: 20 300 °C coefficient: 7.8e-06 K-1 dPgF: -0.0055 climatic_resistance: 3.0 acid_resistance: 53.2 phosphate_resistance: 4.2
Comments
Recommended
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets