Optical constants of OHARA - BSM (Borosilicate, medium-index)
BSM7
Wavelength:
µm
(0.3 – 2.4)
Derived optical constants
n
k
logX
logY
eV
Dispersion formula
$$n^2=2.5432134-0.0102068λ^{2}+0.013983216λ^{-2}+0.00045963235λ^{-4}-3.2963243\text{×}10^{-05}λ^{-6}+1.9413424\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_is_absolute: false λ_is_vacuum: false temperature: 25.0 °C coefficients_of_thermal_dispersion: 2.929e-06 0.0 0.0 0.0 0.0 0.0 n_d: 1.607291 V_d: 59.375631 glass_code: 607594 glass_status: preferred density: 3.51 g/cm3 coefficient_of_thermal_expansion_1: 6.5e-06 K-1 coefficient_of_thermal_expansion_2: 7.6e-06 K-1 ΔP_gF: -0.0017 acid_resistance: 51.2 phosphate_resistance: 2.2
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets