Optical constants of OHARA - BPH (Borophosphate, high-index)
BPH8
Wavelength:
µm
(0.3 – 2.4)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.59323023λ^2}{λ^2-0.0103458172}+\frac{0.277775516λ^2}{λ^2-0.0474089271}+\frac{1.04070526λ^2}{λ^2-81.2863792}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 1.003e-05 0.0 0.0 0.0 0.0 0.0 nd: 1.720467 Vd: 34.716156 glass_code: 720347 glass_status: preferred density: 4.2 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 5.4e-06 K-1 - temperature_range: 20 300 °C coefficient: 6.7e-06 K-1 dPgF: -0.0027 acid_resistance: 53.2 phosphate_resistance: 4.2
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets