Optical constants of OHARA - BAM (Barium, medium-index)
BAM9
Wavelength:
µm
(0.3 – 2.4)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.6446959-0.0094397093λ^{2}+0.018905035λ^{-2}+0.00050396096λ^{-4}-6.9325864\text{×}10^{-06}λ^{-6}+1.5474561\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 4.07e-06 0.0 0.0 0.0 0.0 0.0 nd: 1.643279 Vd: 47.850606 glass_code: 643479 glass_status: preferred density: 3.85 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 6.9e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 8e-06 K-1 acid_resistance: 52.2 phosphate_resistance: 3.2
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets