Optical constants of OHARA - BAL (Barium, low-index)
BAL7
Wavelength:
µm
(0.3 – 2.4)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.4787185-0.0085856348λ^{2}+0.015210012λ^{-2}+0.0006044033λ^{-4}-3.8936391\text{×}10^{-05}λ^{-6}+2.7124338\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 3.871e-06 0.0 0.0 0.0 0.0 0.0 nd: 1.588750 Vd: 51.179278 glass_code: 589512 glass_status: preferred density: 3.18 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 7.5e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 8.8e-06 K-1 dPgF: -0.0012 acid_resistance: 4.2 phosphate_resistance: 2.2
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets