Optical constants of OHARA - BAH (Barium, high-index)
S-BAH54
Wavelength:
µm
(0.3 – 2.4)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.802774-0.011441428λ^{2}+0.023830231λ^{-2}+0.00057322688λ^{-4}+1.1516047\text{×}10^{-05}λ^{-6}+1.2065896\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 8.228e-06 0.0 0.0 0.0 0.0 0.0 nd: 1.695000 Vd: 42.167111 glass_code: 695422 glass_status: preferred density: 3.3 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 6.6e-06 K-1 - temperature_range: 20 300 °C coefficient: 8.1e-06 K-1 dPgF: -0.0039 acid_resistance: 1.0 phosphate_resistance: 1.0
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets