Optical constants of OHARA - BAH (Barium, high-index)
BAH30
Wavelength:
µm
(0.3 – 2.4)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.6543867-0.0084478289λ^{2}+0.022275774λ^{-2}+0.00090008133λ^{-4}-3.5291806\text{×}10^{-05}λ^{-6}+4.7103195\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 2.492e-06 0.0 0.0 0.0 0.0 0.0 nd: 1.650158 Vd: 39.390461 glass_code: 650394 glass_status: preferred density: 3.91 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 9.2e-06 K-1 - temperature_range: 20 300 °C coefficient: 1.05e-05 K-1 dPgF: 0.0015 acid_resistance: 51.2 phosphate_resistance: 2.0
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets