Optical constants of OHARA - APL
S-APL1
Wavelength:
µm
(0.3 – 2.4)
Derived optical constants
n
k
logX
logY
eV
Dispersion formula
$$n^2=2.2762403-0.0096874647λ^{2}+0.0092330378λ^{-2}+0.00038940853λ^{-4}-3.8018733\text{×}10^{-05}λ^{-6}+2.0693225\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 25.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -6.92e-06 1.28e-08 -1.19e-11 4.99e-07 -4.83e-10 0.09 nd: 1.517277 Vd: 69.563209 glass_code: 517696 glass_status: preferred density: 2.59 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 9.6e-06 K-1 - temperature_range: 20 300 °C coefficient: 1.15e-05 K-1 dPgF: 0.0034 climatic_resistance: 2.0 acid_resistance: 1.0 phosphate_resistance: 1.0
References
OHARA Zemax catalog 2017-11-30 (obtained from http://www.ohara-inc.co.jp)
See also OHARA glass data sheets