Optical constants of HIKARI - multiple purpose
5859
Wavelength:
µm
(0.240 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.06973916λ^2}{λ^2-0.00562417858}+\frac{0.422042806λ^2}{λ^2-0.0188055076}+\frac{0.897510953λ^2}{λ^2-71.2142596}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 22.5 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 6.18e-06 1.19e-08 2.91e-13 5.05e-07 1.07e-09 0.118 nd: 1.590421 Vd: 59.473084 density: 2.87 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 4.3e-06 K-1 dPgF: -0.0084 climatic_resistance: 3.0 acid_resistance: 7.0 alkali_resistance: 4.0
References
NIKON Zemax catalog 2017-11 (obtained from http://www.nikon.com)
See also NIKON i-line glass data sheet
Data
INFO
Hikari Glass Co., Ltd.
Hikari Glass Co., Ltd. is a Japanese glass maker, a subsidiary of Nikon Corp.External links
- Hikari Glass Co., Ltd. (in Japanese)
- Nikon