Optical constants of HIKARI - Glasses for precision molding
Q-LAK52S
Wavelength:
µm
(0.280 – 2.400)
Derived optical constants
n
k
logX
logY
eV
Dispersion formula
$$n^2=2.76405609-0.0126400636λ^{2}-0.000160322951λ^{4}+0.0184903089λ^{-2}+0.000267778201λ^{-4}+5.29803264\text{×}10^{-06}λ^{-6}+1.21335917\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 23.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 4.069e-06 1.2323e-08 -1.158e-12 5.3706e-07 5.061e-10 0.17754 nd: 1.677980 Vd: 54.893431 density: 3.55 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 5.9e-06 K-1 dPgF: -0.0074 phosphate_resistance: 4.0
Comments
For mold lens
References
NIKON Zemax catalog 2017-11 (obtained from http://www.nikon.com)
See also HIKARI glass data sheets