Optical constants of HIKARI - SK (Dense crown)
Q-SK5S
Wavelength:
µm
(0.280 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.48684451-0.0107692547λ^{2}-0.000134578724λ^{4}+0.013864428λ^{-2}+0.000124776891λ^{-4}+8.35456207\text{×}10^{-06}λ^{-6}-1.81702443\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 23.0 °C nd: 1.588870 Vd: 61.177645 glass_status: preferred density: 2.93 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 6.8e-06 K-1 dPgF: -0.0036 phosphate_resistance: 4.0
Comments
For mold lens
References
NIKON Zemax catalog 2017-11 (obtained from http://www.nikon.com)
See also HIKARI glass data sheets
Data
INFO
Hikari Glass Co., Ltd.
Hikari Glass Co., Ltd. is a Japanese glass maker, a subsidiary of Nikon Corp.External links
- Hikari Glass Co., Ltd. (in Japanese)
- Nikon