Optical constants of HIKARI - SK (Dense crown)
J-SK16
Wavelength:
µm
(0.290 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.58448044-0.0111132665λ^{2}-0.000137540448λ^{4}+0.0149921982λ^{-2}+0.000188581834λ^{-4}+3.56240422\text{×}10^{-06}λ^{-6}+7.76507396\text{×}10^{-08}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 23.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 9.56742e-07 8.62529e-09 2.05826e-12 4.36559e-07 5.9131e-10 0.172138 nd: 1.620410 Vd: 60.245509 density: 3.56 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 6e-06 K-1 dPgF: -0.0031 phosphate_resistance: 3.0
References
NIKON Zemax catalog 2017-11 (obtained from http://www.nikon.com)
See also HIKARI glass data sheets
Data
INFO
Hikari Glass Co., Ltd.
Hikari Glass Co., Ltd. is a Japanese glass maker, a subsidiary of Nikon Corp.External links
- Hikari Glass Co., Ltd. (in Japanese)
- Nikon